Large and small particles refer to the presence of a certain number of large or small particles in the product. Large particles are particles with a size greater than 5mm in any direction, including connected particles. If your vibrating screen is set to screen out large particles with a mesh size of 8mm, during the operation of the vibrating screen, materials with a diameter of 5~8mm will definitely pass through the vibrating screen and enter the product material.

 

Small particles are defined as particles with a size less than 2mm in any direction, including debris and broken particles. Next, we analyze the reasons for the formation of large and small particles.

 

 
reason
 

 

Template heating temperature

 

Whether the template heating temperature is uniform or not directly affects whether the molten material can smoothly pass through the molding channel of the granulation template. The template used in this device is a hot channel template, and the high-temperature hot oil is heated from the inside to keep the resin in a good molten state. The mold holes are evenly distributed on the template. Only when the discharge speed of each mold hole is consistent can particles of uniform size be cut out.

 

If the temperature control is uneven, the flow rate of the material in some mold holes will be uneven. Under the action of the pelletizing knife disc, irregular particles of different lengths will appear, which will seriously affect the product quality. Because the hot oil system of this device is not a closed design, the hot oil is easy to carbonize during operation. When the hot oil system is running, the carbonized material is easy to block or stick to the flow channel, causing uneven heating; in addition, due to design reasons, the hot oil pipeline is located at a higher position. If the hot oil system is not well sealed, it is easy to inhale air, causing system pressure fluctuations, and it is also easy to cause uneven heating of the template.

 

In addition, when producing low melt flow rate products, the template runs for a long time and the large-aperture filter used will inevitably allow a small amount of carbide to enter the template. Long-term accumulation can easily cause the mold holes to be blocked. When the resin passes through the mold holes, the resistance is different and the speed at which it passes through the mold holes is different, resulting in large and small particles.

 

Cutter

 

Wear or breakage of the cutter can also cause large and small pellets. Whether the cutter feed pressure matches the cutter speed directly affects the length of the pellets and the service life of the cutter. Excessive cutter pressure can lead to cutter breakage accidents, while too low cutter feed pressure can lead to knife padding or even knife entanglement accidents, which seriously affect the quality of pelletizing.

 

The cutter is seriously worn due to the influence of material and process conditions; when operating the extrusion granulator, the load is lifted and lowered too quickly, resulting in large changes in the pressure of the cutter disc and the cutter is easy to break; during the screen changer, the gas inside the screen changer is not discharged cleanly, so that the remaining gas in the screen changer is discharged from the template into the water chamber, resulting in large changes in the pressure of the cutter; these reasons will cause the operation of the pelletizer to deteriorate, the pelletizing is not uniform, and large and small pellets are produced. Among them, when the cutter speed is higher than the material discharge speed, the phenomenon of increasing small pellets will appear. On the contrary, when the cutter speed is lower than the material discharge speed, the phenomenon of increasing large pellets will appear. At present, the cutter speed of this device is controlled at 300~600r/min. Among them, for every increase or decrease of one ton of load, the upper and lower adjustments are 5r/min.

 

Unreasonable cooling water temperature

 

In the start-up procedure of the pelletizing unit, one of the most important factors that determines whether the start-up can be successful is the three simultaneous processes of "water", "knife" and "material". That is, the cooling water enters the water chamber, the pelletizer knife disc rotates, and the template discharges the material. The three processes must be carried out simultaneously to ensure the success of the start-up. Among them, the temperature setting of the cooling water is one of the important factors.

 

After the cooling water enters the water chamber, the template is quickly cooled, especially the lower half of the template is the first to contact the cooling water. If the temperature setting of the cooling water is unreasonable, the mold holes in the lower half of the template may be blocked over a large area. The blocked mold holes are difficult to be flushed open by the polymer in subsequent production, resulting in uneven discharge speed of the template discharge hole, abnormal pelletizing effect, and the formation of "large and small pellets". Unreasonable cooling water temperature will also reduce the service life of the cutter.

 

Other causes

 

When producing polypropylene products with different MFR and rubber content, it is necessary to adjust the operating process parameters of the pelletizer. If the parameters are not set properly, the pelletizer speed and the gap between the cutter and the template are not appropriate, it will also lead to uneven pelletizing and produce large and small pellets.

 

1

 

 
Improvement measures
 

 

Blade pressure control, cooling water temperature control

 

The size of the knife pressure directly determines the quality of the pellet shape. Too much knife pressure will make the pelletizer closer to the template, which will cause the cutter to wear and even break, while too little knife pressure will cause the knife to wrap and pad. Therefore, strict control should be made to keep the knife pressure at (0.2±0.05)MPa.

 

Too low cooling water temperature will cause the die hole of the template to be blocked, while too high temperature will cause tailing and continuous pellets. Therefore, strict control of the cooling water temperature to keep it at 50~65℃ can effectively reduce the formation of large and small pellets.

 

Change the granulation cutter and pH value of cooling water in time

 

The acidity and alkalinity of the cooling water will corrode the back of the cutter blade. Since the cooling water used in this device comes from desalted water, pH=6 is acidic. Therefore, in order to extend the service life of the cutter and avoid the cutter from breaking suddenly during long-term use, the cutter should be monitored more closely and the blade should be replaced in time. You can also add appropriate weak alkali to change the pH of the cooling water to a more neutral pH to reduce the possibility of corrosion.

 

Strengthen daily monitoring and management

 

In order to achieve the control of the appearance quality of the particles, strengthen the inspection of the particle shape during sampling. When sampling granulation, the operator needs to carefully check the appearance of the particles. If there are large and small particles, promptly notify the process and equipment personnel to check and deal with the cutter. At the same time, contact the inspection personnel to review the large and small particles. To strengthen the inspection work, once the large and small particles are found, the process parameters should be adjusted in time and the opening rate should be calculated.

 

(Production rate × number of particles × 1000) ÷ (number of blades × tool speed × 60) = number of unobstructed holes In the formula: production rate unit is kg/h; number of particles unit is g; pelletizer speed is r/min (number of holes ÷ number of mold holes) × 100% = opening rate.